Mô tả
OK 63.30
Extra low carbon stainless steel electrode for welding steelss of the 18Cr 12Ni 2.8Mo-type. Also suitable for welding
of stabilized stainless steels of similar composition, except when the full creep resistance of the base metal is to be met.
Classifications: | EN ISO 3581-A:E 19 12 3 L R 1 2, SFA/AWS A5.4:E316L-17, Werkstoffnummer :1.4430, CSA W48:E316L-17 |
Approvals: | CE EN 13479, BV 316L, DNV 316L, Seproz UNA 272580, GL 4571, NAKS/HAKC
2.5-4.0 mm, ABS SFA/AWS A5:4, E316L-17, CWB CSA W48: E316L-17, DB 30.039.06, LR 316L, VdTÜV 00262 |
Approvals are based on factory location. Please contact ESAB for more information.
Welding Current: | DC+, AC |
Ferrite Content: | FN 3-10 |
Alloy Type: | Austenitic CrNiMo |
Typical Tensile Properties | |||
Condition | Yield Strength | Tensile Strength | Elongation |
ISO | |||
As welded | 460 MPa | 570 MPa | 40 % |
Typical Charpy V-Notch Properties | ||
Condition | Testing Temperature | Impact Value |
ISO | ||
As welded | 20 °C | 60 J |
As welded | -20 °C | 55 J |
As welded | -60 °C | 43 J |
Typical Weld Metal Analysis % | |||||||
C | Mn | Si | Ni | Cr | Mo | N | Ferrite FN |
0.02 | 0.6 | 0.8 | 11.0 | 18.1 | 2.6 | 0.10 | 6 |
Deposition Data | ||||||
Diameter | Current | Voltage | kg weld metal/ kg electrodes | Number of electrodes/kg weld metal | Fusion time per electrode at 90% I max | Deposition rate 90% I max |
1.6 x 300 mm | 30-45 A | 29 V | 0.56 | 250 | 37 s | 0.4 kg/h |
2.0 x 300 mm | 45-65 A | 29 V | 0.60 | 147 | 39 s | 0.6 kg/h |
2.5 x 300 mm | 45-90 A | 29 V | 0.55 | 96 | 45 s | 0.9 kg/h |
3.2 x 350 mm | 60-125 A | 30 V | 0.55 | 52 | 57 s | 1.4 kg/h |
4.0 x 350 mm | 70-190 A | 32 V | 0.56 | 34 | 57 s | 2.0 kg/h |
5.0 x 350 mm | 100-280 A | 32 V | 0.56 | 21 | 63 s | 3.0 kg/h |
Đánh giá